Technical => Roo Man's Room => Topic started by: Mister_Fitz on June 11, 2017, 12:58:52 PM
-
I'm going to change the lower lengthwise tubes in my front engine dragster chassis. There is a small radius and small angel bend on each tube where the engine plate is located.
Which tube bender can you recommend? I should be both affordable and high quality as always...
I have seen an old video from Mark Williams where they are building a RED. At some point in the video they use a gas welder to heat the rubes and bend them into position. It was a bend with small angel. Is this a method still used? How is the tubes like this treatment?
-
we use pro tool bender, the bender is not bad, it's the dies that hurt????????
about 10 years ago we redid a mark Williams car that mark build (fed) yes he used a gas torch to heat the tubes. we had many phone calls with then about that car.
steve m
-
Heat bending is the proper way to do this. "ANY" comercially availble bender will crush the bend into the tube, whether it be a mandrel type or not for just a small bend area, its not as noticable when doing a longer bend.
Its best to mark off a 6" area where the bend will be a heat the area with a "rosebud" tip, keeping a higher percentage of the heat to the inside of the bend because you want to compress the ID over stretching the OD. The longer the sweep 6" vs 2" does not distrupt the material flow and less likely to kink the bend.
It can be tricky, and is why a lot of shops build these "OIL DERRICK" frames instead of being more traditonal
Pro tool, JD Square are junk for doing thin wall moly tubing because its a mandrel action without the mandrel and without it, the OD stretches and deforms the tubing and the bend is "EGG Shaped", do a bend with one of these type, cut the bend in the middle, rotate 180* and try and weld the 2 back together without using any rod
-
Bruce is right on the money on this one. When I was building Ernie Broughton's Comanche clone Don Long (who built the original) was adamant that heat bending was the only acceptable way to do it.
Roo
-
It sounds like heat bending is the way to go.
I have never bent a tube with a gas torch before so every bit of tip or instruction of how to do this with a good result would be very much appreciated.
Would you bend the tube first then welding it to the frame. Or would you weld the first part of the tube to the frame then make the bend and after that weld the rest of the tube to the frame?
-
Even heated, does it need to pack the tubes with sand to avoid crushing?
-
Even heated, does it need to pack the tubes with sand to avoid crushing?
NO, thats why you heat up a 6" section and make it a gradual bend.
-
It sounds like heat bending is the way to go.
I have never bent a tube with a gas torch before so every bit of tip or instruction of how to do this with a good result would be very much appreciated.
Would you bend the tube first then welding it to the frame. Or would you weld the first part of the tube to the frame then make the bend and after that weld the rest of the tube to the frame?
I do both if building a traditional torsion front half. lock the frame down to the table so that the lower rails dont move and insert rail and spot tack. heat and bend til front part fits into a holding fixture and then do the oppiste side. the upper will have to be removable so to be able to fit the upper tube to the lower tube. When stacking the front tubes, where they come to the torsion tube, the width must be greater then the torsion tube so that there is at least 1/4 to 3/8" above and below the torsion tube so that the rails wrap 200* around it for proper welding and support and the cope where the upper and lower tube weld is much shorter instead of if the tubes where to meet the torsion tube the cope and weld would be much much longer
-
Even heated, does it need to pack the tubes with sand to avoid crushing?
NO, thats why you heat up a 6" section and make it a gradual bend.
Thanks Bruce!
-
Are you talking just slight bends in the frame rails or all the bends like roll cage and the back of the seat?
-
^^^^^^^
Just the slight bend required at the mid plate etc. Anything like the cage and shoulder hoop requires an actual tube bender.
Roo
-
Thanks for all the good advices.
Just one more question... :)
Do I need a acetylene and oxygen gas welder or could I get away with a propane/butane (LPG) gas burner?
-
You will need a O/A unit and a rosebud tip torch to heat the tube 360* , you can use propane if you get a roofing torch, but you have to be real careful that you dont overheat the tubing because of the size of the flame it produces